TECAPEEK CM XP91 natural
PEEK compression molded, filled with 30% glass fibre
This compression molded material is a Victrex® PEEK polymer modified with 30% glass fibre for increased strength.
>
| Mechanical properties | Value | Unit | Parameter | Norm |
|---|---|---|---|---|
| Modulus of elasticity (tensile test) |
8200 | MPa | ASTM D 638 | |
| Tensile strength | 89 | MPa | ASTM D 638 | |
| Elongation at break (tensile test) | 2.1 | % | ASTM D 638 | |
| Flexural strength | 144 | MPa | ASTM D 790 | |
| Modulus of elasticity (flexural test) |
6800 | MPa | ASTM D 790 | |
| Shore hardness | 91 | - | Shore D | ASTM D 2240 |
| Thermal properties | Value | Unit | Parameter | Norm |
|---|---|---|---|---|
| Melting temperature | 342 | C | DSC | - |
| Relative costs | Value | Unit | Parameter | Norm |
|---|---|---|---|---|
| Relative costs EU from € to €€€€€€ | €€€€€ |